BONDERITE C-AK 305
Harmonization Code : 3909.20.00.90 | Amino-resins, phenolic resins and polyurethanes, in primary forms : Melamine resins : Other
Main features
- Low-Foam Metal Strip Cleaning
- Continuous Spray-Plant Processing
- Controlled Alkaline Etching
Product Description
BONDERITE C-AK 305 is a concentrated liquid alkaline etching cleaner for aluminum, steel, hot-dip galvanized, and electro-galvanized strip surfaces. Applied in spray-washing equipment, it combines cleaning and controlled etching with low-foam, low-sludge, and minimum-scale behavior. The working bath operates at 40 to 60 deg C with treatment times of 5 to 25 seconds, and substrate-specific bath makeup ranges cover aluminum, steel, and galvanized-strip processing. The formulation is particularly useful in continuous metal-strip plants where bath control and short spray-process cycles are required.
Key features
- Multi-metal strip cleaning: Cleans aluminum, steel, hot-dip galvanized, and electro-galvanized strip.
- Low-foam bath operation: Combines low foam, low sludge, and minimum scale in alkaline etching service.
- Continuous spray processing: Runs at 40 to 60 deg C with 5 to 25 second treatment times.
Applications
Applications include alkaline etching and cleaning of aluminum, steel, hot-dip galvanized, and electro-galvanized strip by spray or continuous-strip processes.
TDS, SDS & Technical Documents
Technical Specifications
General Properties
Thermal Properties
Physical Properties
Additional Information
As-supplied / before-processing properties
Concentrate storage and working-bath makeup and operating parameters.
| Property | Value | Unit | Method / condition |
|---|---|---|---|
| Bath makeup - aluminum | 20 to 40 | L per 1,000 L | Working bath; substrate-dependent |
| Bath makeup - hot-dip galvanized | 10 to 20 | L per 1,000 L | Working bath; substrate-dependent |
| Bath makeup - steel and electro-galvanized | 20 to 40 | L per 1,000 L | Working bath; substrate-dependent |
| Operating temperature | 40 to 60 | deg C | Working bath |
| Treatment time | 5 to 25 | sec | Spray process |
| Recommended storage temperature | 0 to 40 | deg C | Concentrate |
| Shelf life | 24 | months | Unopened original packaging |